 		     			Aanbevelingen
NOELSON™ ZP 409-3, TP-306, NOELSON™ IJzeroxidepigmenten enz.
Formuleringen
2K Epoxy-zinkfosfaat roestwerende primer:
| Deel A | ||
| Epoxyhars | 20 | Epoxy-equivalent: 600-700, Beckopox EP301 (Cytec) | 
| Epoxyhars | 1 | Epoxy-equivalent: 180-200, Beckopox EP116 (Cytec) | 
| 1-Methoxy-2-propanol | 6.2 | Oplosmiddel | 
| BIJK 204 | 0,5 | Bevochtigingsmiddel | 
| methylisobutylketon | 1.5 | Oplosmiddel | 
| Xyleen | 9 | Oplosmiddel | 
| Anti-uithardingsmiddel | 5.2 | 10% Bentone SD-2 in xyleen | 
| F gerookte silica | 0,4 | Reologisch middel | 
| Zinkfosfaat | 6.6 | NOELSON™ ZP 409-3 | 
| Barium sulfaat | 18 | Door Noelson Chemicals | 
| Talk-vuller | 17 | |
| TiO2 | 3.6 | |
| Deel B | ||
| epoxyhars verharder | 11 | Versamid 115 (Cognis) | 
Luchtdroge alkyd-roestwerende primer:
| Alkydhars met lange olie | 400 | |
| Ijzeroxide | 161 | NOELSON™ 130N | 
| Zinkfosfaat | 80 | NOELSON™ ZP 409-3 | 
| Talk-vuller | 96 | |
| Barium sulfaat | 43 | Door Noelson Chemicals | 
| ZnO | 9 | Door Noelson Chemicals | 
| Dispergeermiddel | 2 | |
| Oplosmiddel met hoog kookpunt | 20 | |
| Ethanol-oplosmiddel | 191 | |
| Kobaltdroger, 6% | 6 | |
| Looddroger, 24% | 4 | |
| Anti-vilt | 2 | 
Resultaten van een zoutsproeitest van 400 uur (GB/T 1771-1991):
Controle 6,6% ZP409 6,6% ZP409-1 6,6% ZP409-3
 
         